Next Article in Journal
Interpretation of Nondestructive Magnetic Measurements on Irradiated Reactor Steel Material
Next Article in Special Issue
Cyclic Tests and Numerical Analyses on Bolt-Connected Precast Reinforced Concrete Deep Beams
Previous Article in Journal
New Protocol and Architecture for a Wastewater Treatment System Intended for Irrigation
Previous Article in Special Issue
Flexural Behavior of Reinforced Concrete Beams Retrofitted with Modularized Steel Plates
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Strengthening Design of RC Columns with Direct Fastening Steel Jackets

1
Key Laboratory of Concrete and Prestressed Concrete Structures of the Ministry of Education, Southeast University, Nanjing 210096, China
2
Department of Civil Engineering, The University of Hong Kong, Pokfulam Road, Hong Kong, China
*
Author to whom correspondence should be addressed.
Appl. Sci. 2021, 11(8), 3649; https://doi.org/10.3390/app11083649
Submission received: 1 April 2021 / Revised: 12 April 2021 / Accepted: 14 April 2021 / Published: 18 April 2021
(This article belongs to the Special Issue Seismic Assessment and Retrofit of Reinforced Concrete Structures)

Abstract

:
For non-seismically designed columns with insufficient strength and flexural stiffness, intense inter-story drift can be incurred during a strong earthquake event, potentially leading to the collapse of the entire building. Existing strengthening methods mainly focus on enhancing axial or flexural strength but not the flexural stiffness of columns. In response, a novel direct fastening steel jackets that can increase both flexural strength and stiffness is introduced. This novel strengthening method features straightforward installation and swift strengthening as direct fastening is used to connect steel plates together to form a steel jacketed column. This new connection method can quickly and stably connect two steel components together by driving high strength fasteners into them. In this paper, the design procedure of RC columns strengthened with this novel strengthening method is originally proposed, which includes five steps: (1) estimating lateral load capacity of damaged RC columns; (2) determining connection spacing of steel jacket; (3) estimating the lateral load capacity of strengthened RC column; (4) evaluating the axial load ratio (ALR) of strengthened RC columns; and (5) estimating effective stiffness of strengthened RC columns. Lastly, an example is presented to illustrate the application of the proposed design procedure.

1. Introduction

Reinforced concrete (RC) moment-resisting frame buildings are widely used in schools, hospitals, and residential buildings. RC columns are the principal structural component in the resisting of lateral and gravity loads in frame buildings. Based on post-earthquake investigations [1,2,3], the stability of frame buildings is known to be critically dependent on the seismic performance of RC columns. The structural deficiencies identified in outmoded non-seismically designed RC columns [1,2,3,4,5,6,7,8,9,10] are (1) insufficient lap splice length of longitudinal reinforcement at column ends, (2) insufficient transverse reinforcement at the plastic hinge, (3) strong beam-weak column arrangement, (4) insufficient corrosion resistance, (5) insufficient strength due to new functional use of the building, (6) fire-induced damage, and (7) earthquake-induced damage. The first five above mentioned deficiencies may result in insufficient flexural strength, which can be mitigated by various available strengthening techniques such as RC jacketing [11,12], steel jacketing [13,14] and fiber reinforced polymer (FRP) jacketing [15,16,17]. However, in the case of fire or earthquake damaged columns, both flexural strength and stiffness can be reduced [18,19,20,21]. Figure 1 illustrates the seismic displacement demands of structurally damaged and non-damaged buildings within a demand spectrum. Any reduction in lateral strength and stiffness within a structural system can then induce higher seismic displacement demand during subsequent earthquake events. To restore the seismic capacity of columns to their undamaged state, both flexural stiffness and strength must be improved.
In response, a novel steel jacket that deviates from traditional steel jacketing (assembled by either welding or bolting) is developed (see Figure 2). This new strengthening method offers straightforward installation and rapid strengthening, as direct fastening is used to connect steel plates together to form a steel jacketed column. The strengthening process is briefly described herein: (1) the prefabrication of steel jackets is achieved by welding the end angles to the end of the steel plates (welding can be conducted in-shop); (2) four steel plates are fastened by anchor bolts to the top and base beams; (3) the steel plates are tightly clamped to minimize gaps between them and the RC columns, and steel angles are temporarily fixed to the adjacent steel plates; and (4) the adjacent steel plates and steel angles are tightly and quickly joined by high strength nail using a powder-actuated gun (see Figure 3).
In this paper, previous experimental and theoretical studies on shear connections joined by direct fastening, axial load strengthening and the seismic strengthening of RC columns strengthened by direct fastening steel jackets are first reviewed. Based on the findings in previous studies [22,23,24,25], a design procedure of RC columns strengthened by direct fastening steel jackets is developed. To illustrate the application of the proposed design procedure, a worked example is presented.

2. Review of Previous Work

2.1. Mechanical Behavior of Shear Connectors Joined by Direct Fastening

The connections used in this novel steel jacket resist shear loading incurred as a result of concrete expansion or lateral load. The load transfer process of these connections is similar to that of single lap joints subjected to tensile force at the ends. However, the behaviors of this type of connection have rarely been studied and relevant design specifications are thus not available. Therefore, the experimentation on the single lap joints shown in Figure 4 was carried out to study the mechanical behavior of direct fastening connections [22].
Two kinds of failure modes—bearing and shear fracture—were examined in the tests. Similar to the bearing failure seen in bolted or screwed connections, this failure occurs with enlarged nail holes and bulging of the material around the fastener holes due to large plastic deformation, leading to desirable ductile behavior (see Figure 5).
Although equations for predicting the maximum bearing resistance of bolted and screwed connections are available in current specifications EN-1993-1-8 [26], ANSI/AISC 360-10 [27], and AS 4100 [28], these equations cannot be applied to estimate the maximum bearing resistance (yield strength) of connections joined by direct fastening without modification. Therefore, a unified design equation is developed to evaluate the maximum bearing resistance of the connections:
F b = ψ f p ψ f k α b r d n t p f p u
where αbr is the bearing resistance factor, which is taken as 1.6; ψfp is the factor that considers the effect of protuberance; ψfk is the factor that takes the effect of knurling into account; dn is the nominal fastener diameter; tp is the thickness of the connected steel plate; and fup is the ultimate strength of the connected steel plate.
The two factors caused by the effects of protuberance and knurling are given as:
ψ f p = { 1.35   without   pre - drilled   holes   on   connected   steel   plate 1.0 with   pre - drilled   holes   on   connected   steel   plate
ψ f k = { 1.17   fastener   with   knurling 1.0 fastener   without   knurling

2.2. Axial Strengthening of RC Columns by Direct Fastening Steel Jackets

From the experimental study on the axial strengthening of RC columns by the direct fastening of steel jackets [23], the reliability and effectiveness of the proposed method were observed. Critical parameters (i.e., vertical spacing between adjacent connections, thickness of the steel plate and number of fasteners in each connection) affecting load bearing performance and deformation behavior were identified.
In the proposed strengthening method, steel plates can directly sustain axial load. The axial load contribution of the steel plates is determined by buckling strength as buckling occurs prior to the yield strength of steel plates. The buckling strength is presented in the following section.
Direct fastening connections behave in the manner of transverse reinforcement (i.e., stirrups). Due to the transverse dilation of the column, passive confinement stress is mobilized in stirrups and direct fastening connections, which enhances the strength of the column. To determine confined concrete strength, the equivalent passive confinement stress shown in Equation (3) should be determined.
f e s t = m α s t f y s t A s t s s t l s t
f e d = 2 α d n f F b ( s d + d d ) d c
where m is the stirrup legs; lst is the center-to-center distance of the peripheral stirrup; sst is the stirrup spacing; fyst is the yield strength of the stirrup; Ast is the cross-sectional area of the stirrup; sd is the clear vertical spacing of the adjacent connections; dd is the length of the right steel angle bracket; dc is the column width; αst is the stress ratio of the stirrup; and αd is the shear force ratio of the direct fastening connection.
A theoretical study was carried out to examine the stress ratio of the stirrup and the shear force ratio of the direct fastening connection [24]. Based on an extensive parameter study, a lower bound value of 0.34 is used to represent the stress ratio of the stirrups with a yield strength of 400 MPa. To consider the effect of the yield strength, a yield strength factor of γfyst was proposed. The yield strength factors for yield strengths of 500 MPa and 600 MPa are 0.8 and 0.66, respectively. The shear force ratio of the connections is obtained using:
α d = γ n f ( 0.82 0.64 λ d )
where λd is the normalized connection spacing (λd = sd/dc); and γnf represents a factor of the number of fasteners on the shear force ratio of the connections. When the number of fasteners is 2 and 4, the factor is equal to 0.72 and 0.47, respectively.
The failure criterion proposed in [29] is used to derive the confined concrete strength of fcc′. The failure criterion is given by:
τ o c t * = 6.9638 ( 0.09 σ o c t * c σ o c t * ) 0.9297
c = 12.2445 ( cos 1.5 θ ) 15 + 7.3319 ( sin 1.5 θ ) 2
cos θ = 3 2 s 1 J 2
τ o c t * = τ o c t f c
σ o c t * = σ o c t f c
where τoct and σoct are the octahedral shear and normal stress, respectively; θ is the direction of the deviatoric stress on the deviatoric plane; s1 is the first deviatoric stress; J2 represents the second invariant of the deviatoric stress tensor; and fc′ is the compressive strength of the unconfined concrete.
The key parameters in the applied failure criterion are summarized as follows:
s 1 = f c c f 3
J 2 = 1 3 ( f c c f ) 2
cos θ = f c c f 3 2 τ o c t
τ o c t = 2 ( f c c f ) 3
σ o c t = 2 f + f c c 3
where fcc′ is the axial compressive strength of the confined concrete and f′ is the equivalent passive confinement stress.

2.3. Seismic Strengthening of RC Columns by Direct Fastening Steel Jackets

To investigate the seismic performance of strengthened RC columns using direct fastening steel jackets, an experimental study was conducted [25]. Attention was given to the enhancement of flexural stiffness and strength.
On the basis of comparisons between predicted and measured effective flexural stiffness, the expressions recommended in EN 1994-1-1 [30] are advised to calculate effective flexural stiffness:
K i = ( E I ) s + 0 . 6 ( E I ) c
where (EI)s is the flexural stiffness provided by the steel jacketing; and (EI)c is the flexural stiffness provided by the RC column.
Buckling of the steel plate on the compressive side was observed. The corresponding buckling stress of steel plate under a compressive state should thus be embedded within the theoretical model used to predict lateral capacity. Using the Rayleigh–Ritz method and assuming the initial bowing and subsequent deflection as a trigonometric function, the buckling strength of steel plate is given as:
σ p , c r i t i c a l = 4 π 2 D d p s d 2 A p ( 1 α i )
where D is the bending stiffness of the steel plate per unit width; dp is the plate depth; Ep and μp are elastic modulus and Poisson’s ratio of steel plate; Ap is the cross-sectional area of steel plate; and αi is the imperfection factor.
The imperfection factor αi is introduced to consider the initial bowing effect induced by the welding and is calibrated using the experimental results:
α i = 1 . 046 0 . 73 λ s r 100
where λsr = sd/tp is the slenderness ratio of steel plate. As the empirical imperfection factor was calibrated with limited available data, it is useful to assume a slenderness ratio of the steel plate between 14 and 39.
It is worth noting that the steel plate detached from the RC column at the bottom of the tension fiber. This was largely due to the strain incompatibility between RC column and the steel jacket on the tension side during bending. As a result, the assumption that the plane section would remain plane after deformation throughout the entire length of the column is inaccurate. Hence, a reduction factor of ηi = 0.6 was introduced for the tensile component of the steel plate when the lateral resistant capacity was estimated.

3. Design Procedure

In this section, the critical parameters (i.e., steel plate thickness, fastener number and connection spacing) are first roughly determined. The feasibility of these parameters are further examined by satisfying four conditions: (1) desirable flexural failure occurs prior to brittle shear failure; (2) lateral load capacity is larger than lateral load demand; (3) ALR does not exceed the limit stipulated in current specification; and (4) effective flexural stiffness should be comparable to that of the undamaged RC column.

3.1. Estimating Lateral Load Capacity of Damaged RC Columns

The deficiency of the RC column may occur for a variety of reasons (e.g., fire). It is necessary to estimate the lateral load capacity of the damaged RC column and compare this with the load demand. According to the assumption that the plane section remains plane after deformation, the strain profile and the stress of the longitudinal rebar can be defined (Figure 6).
{ f y l σ l 1 = E s ( d c c ϕ s t ϕ l 2 x c ) ε c u x c f y l f y l σ l j = E s ( d c c ϕ s t ϕ l 2 ( j 1 ) s l x c ) ε c u x c f y l f y l σ l m = E s ( d c c ϕ s t ϕ l 2 ( m 1 ) s l x c ) ε c u x c f y l
where sl is the longitudinal rebar spacing; subscript lj represents the jth row longitudinal rebar counting from the tensile sides (1 ≤ jm); m is the total rows of longitudinal rebars which is equal to the stirrup legs; ϕl is the diameter of the longitudinal rebar; ϕst is the diameter of the stirrup; c is the cover thickness of the column; xc is the compressive depth of the column; εcu is the ultimate strain of concrete and is taken as 0.003 in accordance with ACI 318 [31]; fyl is the yield strength of the longitudinal reinforcement; and σlj is the stress of the jth row longitudinal rebar.
The stress profile of the concrete is quantified using the equivalent rectangular stress block. The compressive depth is then determined by the axial equilibrium:
N 0 + j = 1 m k j A l σ l j γ s α f c d c β x c γ c = 0
where kj is the number of the jth row longitudinal rebar; γs is the partial safety factor of rebar; γc is the partial safety factor of concrete; N0 is the axial load; Al is the cross-sectional area of longitudinal rebar; fc′ is the concrete strength; and α and β are the two factors used to determine the equivalent rectangular stress block.
By taking moment to the extreme compressive fiber of the RC column, the moment capacity is given as:
M c a p = N 0 d c 2 + j = 1 m k j A l σ l j ( d c c ϕ s t ϕ l 2 ( j 1 ) s l ) γ s α f c d c β x c β x c 2 γ c
Under the assumption that the stiffness of the upper and lower joints is comparable, the lateral load resistance is then given by:
V c a p = M c a p 0 . 5 L    
where L is the length of the column.
If lateral load capacity cannot satisfy lateral load demand, the RC column can be strengthened using the direct fastening steel jackets.

3.2. Determining Connection Spacing of Steel Jacket

Flexural failure is the desirable failure mode. To ensure that desirable flexural failure occurs, the following relationship should be satisfied in light of ASCE 41-13 [32].
V V c a p , s t r e n 0.6 V s t r e n
where V is the lateral load demand acting on the RC column; Vcap,stren is the lateral load corresponding to the moment capacity of the strengthened RC column; and Vstren is the shear strength of the strengthened RC column which is determined by the following expression:
V s t r e n = V d + V c + V s = 0.5 d c s d + d d 2 n f F b γ s + 0.17 ( 1 + N 0 14 A c ) f c d c d w γ c + m A s t f y s t d w γ s s s t
where nf is the fastener number in a connection; Ac is the cross-sectional area of the column; and dw is the depth of the column.
The first term represents the shear resistance produced from the connections. To avoid an overestimation of the shear resistance from the steel jacket, a factor of 0.5 is introduced by following EN 1998-3:2005 [33]. As the partial safety factor for direct fastening connections is absent, the partial safety factor of steel rebar is used.
Combining the above two expressions, the connection spacing of the steel jacket can be determined.

3.3. Estimating Lateral Load Capacity of Strengthened RC Column

According to the assumption that the plane section remains plane after deformation, the strain profile and stress profile of the longitudinal rebar and steel plates of the strengthened RC column are defined, respectively (see Figure 7). It should be noted that the side plate is divided into n equal small parts to accurately define the stress in the side plate. Moreover, the buckling of the steel plate under a compressive state is embedded.
{ σ p t = E p ( d c + t p 2 x c ) ε c u x c f p y σ p c = E p ( t p 2 + x c ) ε c u x c σ p , c r i t i c a l σ p , c r i t i c a l σ p s i d e _ i = E p ( d c d c d p 2 Δ i 2 ( i 1 ) Δ i x c ) ε c u x c f p y f y l σ l 1 = E s ( d c c ϕ s t ϕ l 2 x c ) ε c u x c f y l f y l σ l j = E s ( d c c ϕ s t ϕ l 2 ( j 1 ) s l x c ) ε c u x c f y l f y l σ l m = E s ( d c c ϕ s t ϕ l 2 ( m 1 ) s l x c ) ε c u x c f y l
where i represents the ith partitioned part of the steel plate parallel to the lateral load counting from the tensile side; σpside_i is the stress of the ith partitioned part of the steel plate parallel to the lateral load; Δi is the length of the equal small part and is equal to dp/n; and σp,critical is the ultimate compressive stress of the steel plate, which can be defined by Equation (8).
The compressive depth of the strengthened RC column is then determined by the axial equilibrium.
0 = N 0 + j = 1 m k j A l σ l j γ s + η i σ p t A p A p σ p c + 2 i = 1 n t p Δ i σ p s i d e _ i γ s α f c d c β x c γ c
By taking moment to the extreme compressive fiber of the strengthened RC column, the moment capacity is given as:
M c a p , s t r e n = N 0 d c 2 α f c d c β x c β x c 2 γ c + j = 1 m k j A l σ l j ( d c c ϕ s t ϕ l 2 ( j 1 ) s l ) γ s + η i σ p t A p ( d c + t p 2 ) + A p σ p c t p 2 + 2 i = 1 n t p Δ i σ p s i d e _ i ( d c d c d p 2 Δ i 2 ( i 1 ) Δ i ) γ s
Under the assumption the stiffness of the upper and lower joints is comparable, the lateral load resistance is then given by:
V c a p , s t r e n = M c a p , s t r e n 0 . 5 L    
Then, the relationship between the ultimate lateral load and the lateral load resistance of the strengthened RC column can be checked.

3.4. Estimating ALR of Strengthened RC Columns

The confined concrete divisions are shown in Figure 8a. Confined concrete 1 is confined by the erected steel jacket. Confined concrete 2 is confined by the stirrup. Confined concrete 3 is confined by the stirrup and erected steel jacket. Because the area of confined concrete 1 and confined concrete 2 is relatively smaller than that of confined concrete 3, and these two areas are close, the confined concrete divisions can be simplified in the design calculation. The simplified concrete divisions are shown in Figure 8b, in which the confined effect of confined concrete 2 is imposed on confined concrete 1. Thus, the initial three varieties of confined concrete can be equivalent to one confined concrete that is confined by a stirrup and steel jacket. For the confined concrete in Figure 8b, the imposed equivalent passive confinement stress is fl = fest + fed, which can be determined according to (3). Using the confined concrete strength model in (5), the confined concrete strength (fcc′) can be determined. Thus, the axial load capacity is given as:
N c , s t r e n = A c c f c c + A c 0 f c γ c + ( 4 m 4 ) A l f y l + 4 P p , c r i t i c a l γ s
where Acc is the area of confined concrete in Figure 8b; and Ac0 is the area of the unconfined concrete in Figure 8b.
The confined concrete area Acc and unconfined area Ac0 are respectively given as:
A c c = d c 2 4 d l 2 6 ( 4 m 4 ) A l
A c 0 = 4 d l 2 6
where dl is the edge-to-edge horizontal distance of the connections, as shown in Figure 8b.
The ALR is given as:
ALR = N 0 N c , s t r e n
According to the recommendation in EN 1998-1:2004 [34], the ALR must necessarily be less than 0.65.

3.5. Estimating Effective Stiffness of Strengthened RC Columns

In light of the findings relating to the seismic strengthening of RC columns by direct fastening steel jackets, the effective flexural stiffness of the strengthened RC column can be estimated by (7). The effective flexural stiffness of the strengthened RC column should be comparable to that of the undamaged RC column, with the aim of the deformation capacity and seismic load carrying capacity remaining unchanged.

4. Parameter Study

A parameter study is conducted in this section to investigate the enhancement ratio (ηM = Vcap,stren/ Vcap) of the lateral load capacity of strengthened RC columns and roughly estimate the required thickness of steel plate. Four critical variables (i.e., thickness of steel plate, cross-sectional dimension of column, longitudinal rebar ratio ρl and ALR) are investigated to plot the design curves. The range of these four variables is set out in Table 1. The yield strength and elastic modulus of the longitudinal rebar are 500 MPa and 200 GPa, respectively. The yield strength, ultimate strength and elastic modulus of the steel plate are 300 MPa, 400 MPa and 200 GPa, respectively. The cylinder strength of the concrete is 30 MPa. The compressive strength of the compressive steel plate is greatly affected by its slenderness ratio (λsr). For conservative consideration, λsr is taken as 38, which is the upper bound value of the slenderness ratio of steel plate determined from the experimental study [23,25].
It can be determined from Figure 9 that the enhancement ratio is significantly affected by the thickness of the steel plate and longitudinal rebar ratio. The enhancement ratio increases with the thickness of the steel plate, which can be seen from Equation (17). The enhancement ratio declines by 20% when the longitudinal rebar ratio increases from 0.015 to 0.03, as RC columns comprised of more longitudinal rebar possess a higher lateral load capacity, causing the decreased enhancement ratio. Compared with the effect of the longitudinal rebar ratio, the effect of the ALR on the enhancement ratio is marginal, especially for RC columns possessing higher longitudinal rebar ratios.

5. Worked Example

The prototype of the RC column is shown in Figure 10. The height of the column is 3000 mm. The cross-sectional dimension is 500 mm × 500 mm. The reinforcement cage is formed by 12T20 and R10@150. At the ultimate limit state, the factored axial load (N0) and factored lateral load (V) are 1400 kN and 300 kN, respectively. The elastic modulus of the rebar is 200 GPa. The yield strength of the stirrup and the longitudinal rebar is 400 MPa and 500 MPa, respectively. The cylinder strength (fc′), cube strength (fcu), and elastic modulus (Ec) of the concrete are 30 MPa, 40 MPa, and 25 GPa, respectively. The cover thickness (c) is 20 mm. It is postulated that the column experienced a fire event up to 570 °C. The strength and stiffness of the RC column can be greatly impaired after exposure to high temperature. The proposed strengthening method of directly fastening steel jackets can be used to restore fire-damaged RC columns. The elastic modulus, yield strength and ultimate strength of the steel plate are 200 GPa, 300 MPa and 400 MPa, respectively. The steel angle bracket used to connect the two adjacent steel plates measures 75 mm × 75 mm × 5 mm with a length of 50 mm. The 4 mm diameter high strength knurled fastener is used in this strengthening system. The partial safety factor of steel and concrete is taken as 1.2 and 1.5.

5.1. Evaluating Lateral Load Capacity of Fire-Damaged Column

After the concrete is exposed to fire, the concrete strength is impaired. The concrete strength post fire can be estimated according to the recommendation in EN-1992-1-2 [35]. The residual cylinder strength (fc,pf) of the RC column following exposure to 570 °C fire is 0.5fc′.
According to the study on the mild steel post fire in [22], the residual strength and elastic modulus of rebar can be readily determined. The residual strength of longitudinal rebar is given as:
f y l , p f = f y l R s y =   500 × ( 1.0 0.2 × 570 400 600 ) = 470   MPa
The residual strength of the stirrup is given as:
f y s t , p f = f y s t R s y =   400 × ( 1.0 0.2 × 570 400 600 ) = 376   MPa
The residual elastic modulus of rebar is given as:
E s , p f = E s R s E =   200 × ( 1.0 0.07 × 570 350 500 ) = 194   GPa
According to (20) and (21), the stresses of the four rows of longitudinal rebar and thus the compressive height of the plane section can be determined.
N 0 + 4 A l σ l 1 + 2 A l σ l 2 + 2 A l σ l 3 + 4 A l σ l 4 1.2 α f c , p f d c β x c 1.5 = 0
The compressive height of the plane section is solved as:
x c = 304   mm
The moment capacity is derived by (22).
M c a p = N 0 d c 2 α f c , p f d c β x c β x c 2 1.5   + 4 A l σ l 1 ( d c c ϕ s t ϕ l 2 ) + 2 A l σ l 2 ( d c c ϕ s t ϕ l 2 s l ) 1.2   + 2 A l σ l 3 ( d c c ϕ s t ϕ l 2 2 s l ) + 4 A l σ l 4 ( d c c ϕ s t ϕ l 2 3 s l ) 1 . 2 = 311   kN m
The lateral load resistance of the fire-damaged RC column is given by (23).
V c a p = M c a p 0.5 L   =   311 × 10 3 0.5 × 3000   =   207   kN   <   V = 300   kN
Thus, the fire-damaged RC column is not safe, and the required enhancement ratio of the RC column is around 1.4.

5.2. Evaluating Lateral Load Capacity of Strengthened RC Column

Since the required enhancement ratio is around 1.4 and the longitudinal rebar ratio is 0.015, 4 mm steel plate is utilized to strengthen the fire-damaged RC column based on the findings in Figure 8. Additionally, four fasteners on the connection are used.
(a)
Determining connection spacing
Flexural failure is the desirable failure mode. To realize this, Equation (24) should be satisfied.
300   kN   =   V V c a p , s t r e n 0.6 V s t r e n
According to Equation (25), the shear capacity of the strengthened fire-damaged RC column is given as:
V s t r e n = V d + V c , p f + V s , p f = 0.5 d c s d + d d 2 n f F d γ s + 0.17 ( 1 + N 0 14 A c ) f c , p f d c d w γ c + m A s t f y s t , p f d w γ s s s t = 0.5 × 500 s d × 2 × 4 × 1.6 × 1.35 × 1.17 × 4 × 4 × 400 1.2 + 0.17 ( 1 + 1400 × 1000 14 × 500 × 500 ) 1 . 5   × 15 × 500 × ( 500 c ϕ s t ϕ l 2 ) + 4 × 3.14 × 10 2 4 × 376 × ( 500 c ϕ s t ϕ l 2 ) 150 × 1 . 2
Solving the above two equations, the connection spacing is given as:
s d 160   mm
Here, the connection spacing is taken as 100 mm. The corresponding shear capacity of the strengthened column is 623 kN.
(b)
Determining ultimate compressive stress in compressive steel plate
The slenderness ratio of the steel plate is given as:
λ s r = s d t p = 100 4 = 25
The initial imperfection factor is given by (19).
α i = 1.046 0.0073 λ s r = 1.046 0.0073 × 25 = 0.86
The ultimate compressive stress of the steel plate is determined by (18).
σ p , c r i t i c a l = 4 π 2 D d p s d 2 A p ( 1 α i ) = 4 π 2 E p t p 2 12 s d 2 ( 1 μ p 2 ) ( 1 α i ) = 4 × 3.14 2 × 200 × 10 3 × 4 2 12 × 100 2 × ( 1 0.3 2 ) × ( 1 0.86 ) = 162   MPa   <   f y p = 300   MPa
(c)
Determining lateral load capacity of strengthened RC column
The stresses in steel plate and longitudinal rebar are given by Equation (26). The compressive depth of the strengthened fire-damaged RC column is determined by Equation (27).
0 = N 0 + 4 A l σ l 1 + 2 A l σ l 2 + 2 A l σ l 3 + 4 A l σ l 4 1.2 + 0.6 σ p t 1 A p A p σ p c 1 + 2 i = 1 n t p Δ i σ p s i d e _ i 1.2 α f c , p f d c β x c 1.5
The compressive height of the plane section of the strengthened fire-damaged RC column is solved as:
x c = 302   mm
The moment capacity of the strengthened fire-damaged RC column is derived by Equation (28).
M c a p , s t r e n = N 0 d c 2 α f c , p f d c β x c β x c 2 1 . 5   + 4 A l σ l 1 ( d c c ϕ s t ϕ l 2 ) + 2 A l σ l 2 ( d c c ϕ s t ϕ l 2 s l ) 1 . 2   + 2 A l σ l 3 ( d c c ϕ s t ϕ l 2 2 s l ) + 4 A l σ l 4 ( d c c ϕ s t ϕ l 2 3 s l ) 1 . 2   + 0.6 σ p t 1 A p ( d c + t p 2 ) + A p σ p c 1 t p 2 + 2 i = 1 n t p Δ i σ p s i d e _ i ( d c d c d p 2 Δ i 2 ( i 1 ) Δ i ) 1 . 2 = 530   kN m
The lateral load resistance of the strengthened fire-damaged RC column is given by Equation (29).
V c a p , s t r e n = M c a p , s t r e n 0.5 L   =   530 × 10 3 0.5 × 3000   =   353   kN   >   V = 300   kN
The condition in (24) is rechecked herein.
V c a p , s t r e n = 353   kN   <   0.6 V s t r e n = 374   kN

5.3. Checking ALR

(a)
Estimating equivalent passive confinement stress
The equivalent passive confinement stress originated from the stirrup and the connections are respectively given by (4) and (5).
f e s t = 4 α s t f y s t , p f A s t s s t l s t = 4 × 0.34 × 376 × 3.14 × 10 2 4 150 × ( 500 20 × 2 10 ) = 0.59   MPa f e d = 2 α d n f F d ( s d + d d ) d c = 2 × 0.47 × ( 0.82 0.64 × 100 500 ) × 4 × 1.6 × 1.35 × 1.17 × 4 × 4 × 400 150 × 500 = 0.56   MPa
(b)
Estimating axial load capacity
For the confined concrete in Figure 7b, the imposed equivalent passive confinement stress is fl = fest + fed = 0.59 + 0.56 = 1.15 MPa. Using the confined concrete strength model in (7)–(16), the confined concrete strength is 22.5 MPa. Thus, the axial load capacity is given by Equations (30)–(32).
N c , s t r e n = A c c f c c , p f + A c 0 f c , p f γ c + 12 A l f y l , p f + 4 A p σ p , c r i t i c a l γ s = ( 500 × 500 12 × 3.14 × 20 2 4 2 3 ( 500 70 × 2 ) 2 ) × 22 . 5 + 2 3 ( 500 70 × 2 ) 2 × 15 1.5   +   12 × 3.14 × 20 2 4 × 470 + 4 × 4 × 495 × 162 1.2 = 5800   kN
The ALR is given by (33).
ALR = N 0 N c , s t r e n = 1400 5800 = 0.24 < 0.65

5.4. Checking Effective Flexural Stiffness

Based on the study conducted by Hwang et al. [6], the residual elastic modulus of concrete retains around 0.2Ec after exposure to a 570 °C fire event. According to (17), the effective flexural stiffness of the strengthened RC column is given as:
K i = ( E I ) s + 0.6 ( E I ) c , p f = 2 E P t p d p 3 12 + E P t p d p d c 2 2 + 0.6 0.2 E c d c 4 12 = 2 × 200000 × 4 × 495 3 12 + 200000 × 4 × 495 × 500 2 2 + 0.6 × 0.2 × 25000 × 500 4 12 = 8.1 × 10 13 N mm 2 7.8 × 10 13 N mm 2 = 0.6 × 25000 × 500 4 12 = 0 . 6 ( E I ) c
Until then, the parameters of the steel jacket (i.e., steel plate thickness, fastener number and connection spacing) are determined. The strengthening scheme is shown in Figure 11.

6. Conclusions

In this paper, a novel direct fastening steel jacket is introduced. The main findings of the available experimental and theoretical studies on the proposed strengthening method are reviewed, based on which the design procedure for the proposed strengthening method is presented. The design procedure can be processed by the application of four critical steps: (1) sizing the steel plate thickness based on the required enhancement ratio and Figure 9; (2) sizing the connection spacing and fastener number by avoiding flexural failure; (3) checking lateral load demand and capacity; and (4) checking the ALR limit. If either of the final two checking conditions is not satisfied, the process should be repeated from step (1) until these two final conditions are satisfied. Subsequently, the effective flexural stiffness is examined to ensure it is similar to that of the undamaged RC column.

Author Contributions

Conceptualization, Z.S. and R.K.L.S.; methodology, Z.S. and R.K.L.S.; investigation, L.C. and K.L.; writing—original draft preparation, Z.S.; writing—review and editing, Z.S., R.K.L.S. and Z.X. All authors have read and agreed to the published version of the manuscript.

Funding

This research was supported by the Fundamental Research Funds for the Central Universities.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The results presented in this study are available on request from the corresponding author.

Acknowledgments

This research was supported by the Fundamental Research Funds for the Central Universities. The authors would like to thank for their financial support.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Free, M.; Rossetto, T.; Peiris, N.; Taucer, F.; Zhao, B.; Koo, R.; Wang, J.; Ma, X.; Verrucci, E. The Wenchuan earthquake of May 12, 2008: Field observations and recommendations for reconstruction. In Proceedings of the 14th World Conference on Earthquake Engineering, Beijing, China, 12–17 October 2008. [Google Scholar]
  2. Li, B.; Wang, Z.; Mosalam, K.M.; Xie, H.P. Wenchuan earthquake field reconnaissance on reinforced concrete framed buildings with and without masonry infill walls. In Proceedings of the 14th World Conference on Earthquake Engineering, Beijing, China, 12–17 October 2008. [Google Scholar]
  3. Sezen, H.; Whittaker, A.S.; Elwood, K.J.; Mosalam, K.M. Performance of reinforced concrete buildings during the August 17, 1999 Kocaeli, Turkey earthquake, and seismic design and construction practise in Turkey. Eng. Struct. 2003, 25, 103–114. [Google Scholar] [CrossRef]
  4. Bousias, S.; Spathis, A.L.; Fardis, M.N. Seismic retrofitting of columns with lap splices through CFRP jackets. In Proceedings of the 13th World Conference on Earthquake Engineering, Vancouver, BC, Canada, 1–6 August 2004. [Google Scholar]
  5. Su, R.K.L.; Lam, N.T.K.; Tsang, H.H. Seismic drift demand and capacity of nonseismically designed buildings in Hong Kong. Electron. J. Struct. Eng. 2008, 8, 110–120. [Google Scholar]
  6. Hwang, E.; Kim, G.; Choe, G.; Yoon, M.; Gucunski, N.; Nam, J. Evaluation of concrete degradation depending on heating conditions by ultrasonic pulse velocity. Constr. Build. Mater. 2018, 171, 511–520. [Google Scholar] [CrossRef]
  7. Anagnostou, E.; Rousakis, T.C.; Karabinis, A.I. Seismic retrofitting of damaged rc columns with lap-spliced bars using frp sheets. Compos. Part B Eng. 2019, 166, 598–612. [Google Scholar] [CrossRef]
  8. Al-Harthy, A.S.; Stewart, M.G.; Mullard, J. Concrete cover cracking caused by steel reinforcement corrosion. Mag. Concrete Res. 2011, 63, 655–667. [Google Scholar] [CrossRef] [Green Version]
  9. Shan, Z.W.; Su, R.K.L. Improved uncoupled closed-form solution for adhesive stresses in plated beams based on Timoshenko beam theory. Int. J. Adhes. Adhes. 2019, 96, 102472. [Google Scholar] [CrossRef]
  10. Shan, Z.W.; Su, R.K.L. Flexural capacity model for RC beams strengthened with bolted side-plates incorporating both partial longitudinal and transverse interactions. Eng. Struct. 2018, 168, 44–57. [Google Scholar] [CrossRef]
  11. Chang, S.Y.; Chen, T.W.; Tran, N.C.; Liao, W.I. Seismic retrofitting of RC columns with RC jackets and wing walls with different structural details. Earthq. Eng. Eng. Vib. 2014, 13, 279–292. [Google Scholar] [CrossRef]
  12. Vandoros, K.G.; Dritsos, S.E. Concrete jacket construction detail effectiveness when strengthening RC columns. Constr. Build. Mater. 2008, 22, 264–276. [Google Scholar] [CrossRef]
  13. Garzon-Roca, J.; Ruiz-Pinilla, J.; Adam, J.M.; Calderón, P.A. An experimental study on steel-caged RC columns subjected to axial force and bending moment. Eng. Struct. 2011, 33, 580–590. [Google Scholar] [CrossRef]
  14. Wang, L.; Su, R.K.L.; Cheng, B.; Li, L.Z.; Shan, Z.W. Seismic behavior of preloaded rectangular RC columns strengthened with precambered steel plates under high axial load ratios. Eng. Struct. 2017, 152, 683–697. [Google Scholar] [CrossRef]
  15. Lam, L.; Teng, J.G. Strength models for fiber-reinforced plastic-confined concrete. J. Struct. Eng. 2002, 128, 612–623. [Google Scholar] [CrossRef]
  16. Demers, M.; Neale, K.W. Confinement of reinforced concrete columns with fibre-reinforced composite sheets—An experimental study. Can. J. Civil. Eng. 1999, 26, 226–241. [Google Scholar] [CrossRef]
  17. Yaqub, M.; Bailey, C.G.; Nedwell, P. Axial capacity of post-heated square columns wrapped with FRP composites. Cem. Concr. Comp. 2011, 33, 694–701. [Google Scholar] [CrossRef]
  18. Wang, L.; Su, R.K.L. Repair of fire-exposed preloaded rectangular concrete columns by postcompressed steel plates. J. Struct. Eng. 2014, 140, 04013083. [Google Scholar] [CrossRef] [Green Version]
  19. Lin, C.H.; Tsay, C.S. Deterioration of strength and stiffness of reinforced concrete columns after fire. J. Chin. Inst. Eng. 1990, 13, 273–283. [Google Scholar] [CrossRef]
  20. Vieira, J.P.B.; Correia, J.R.; De Brito, J. Post-fire residual mechanical properties of concrete made with recycled concrete coarse aggregates. Cem. Concr. Res. 2011, 41, 533–541. [Google Scholar] [CrossRef]
  21. Hyland, C.; Smith, A. CTV Building Collapse Investigation; Department of Building and Housing: Christchurch Central City, New Zealand, 2012. [Google Scholar]
  22. Shan, Z.W.; Su, R.K.L. Behavior of shear connectors joined by direct fastening. Eng. Struct. 2019, 196, 109321. [Google Scholar] [CrossRef]
  23. Shan, Z.W.; Su, R.K.L. Axial strengthening of RC columns by direct fastening of steel plates. Struct. Eng. Mech. 2021, 77, 705–720. [Google Scholar]
  24. Shan, Z.W.; Looi, D.T.W.; Su, R.K.L. Confinement model of RC columns strengthened by direct fastening of steel plate. Steel Compos. Struct. 2021. accepted. [Google Scholar]
  25. Shan, Z.W.; Looi, D.T.W.; Su, R.K.L. A novel seismic strengthening method of RC columns confined by direct fastening steel plates. Eng. Struct. 2020, 218, 110838. [Google Scholar] [CrossRef]
  26. EN-1993-1-8. Design of Steel Structure. Part 1.8: Design of Joints; European Committee for Standardization: Brussels, Belgium, 2005. [Google Scholar]
  27. ANSI/AISC 360-16. Specification for Structural Steel Buildings; American Institute of Steel Construction: Chicago, IL, USA, 2016. [Google Scholar]
  28. AS 4100. Steel Structures; Standards: Sydney, Australia, 1998. [Google Scholar]
  29. Guo, Z.H.; Wang, C.Z. Investigation of strength and failure criterion of concrete under multi-axial stresses. Chin. Civil. Eng. J. 1991, 24, 1–14. [Google Scholar]
  30. EN 1994-1-1:2004. Design of Composite Steel and Concrete Structures. Part 1 1: General Rules and Rules for Buildings; European Committee for Standardization: Brussels, Belgium, 2004. [Google Scholar]
  31. ACI Committee 318. Building Code Requirements for Structural Concrete (ACI 318M-14) and Commentary (ACI 318RM-14); American Concrete Institute: Farmington Hills, MI, USA, 2015. [Google Scholar]
  32. ASCE/SEI 41-13. Seismic Evaluation and Retrofit of Existing Buildings; ASCE Standard: Reston, VI, USA, 2014. [Google Scholar]
  33. EN 1998-3:2005. Design of Structures for Earthquake Resistance—Part 3: Assessment and Retrofitting of Buildings; European Committee for Standardization: Brussels, Belgium, 2005. [Google Scholar]
  34. EN 1998-1:2004. Design of Structures for Earthquake Resistance—Part 1: General Rules, Seismic Actions and Rules for Buildings; European Committee for Standardization: Brussels, Belgium, 2004. [Google Scholar]
  35. EN 1992-1-2. Eurocode 2: Design of Concrete Structures—Part 1–2: General Rules—Structural Fire Design; European Committee for Standardization: Brussels, Belgium, 2004. [Google Scholar]
Figure 1. Design spectrum and capacity curves for damaged and undamaged structures.
Figure 1. Design spectrum and capacity curves for damaged and undamaged structures.
Applsci 11 03649 g001
Figure 2. Proposed strengthening scheme: (a) front view; (b) plane view.
Figure 2. Proposed strengthening scheme: (a) front view; (b) plane view.
Applsci 11 03649 g002
Figure 3. Strengthening procedure.
Figure 3. Strengthening procedure.
Applsci 11 03649 g003
Figure 4. Illustration of connection test joined by direct fastening.
Figure 4. Illustration of connection test joined by direct fastening.
Applsci 11 03649 g004
Figure 5. Mechanical behavior of connections: (a) bearing failure; (b) shear load versus displacement curve.
Figure 5. Mechanical behavior of connections: (a) bearing failure; (b) shear load versus displacement curve.
Applsci 11 03649 g005
Figure 6. Vertical strain and stress profiles of RC column: (a) strain profile; (b) stress profile.
Figure 6. Vertical strain and stress profiles of RC column: (a) strain profile; (b) stress profile.
Applsci 11 03649 g006
Figure 7. Vertical strain and stress profiles of strengthened RC column: (a) strain profile; (b) stress profile.
Figure 7. Vertical strain and stress profiles of strengthened RC column: (a) strain profile; (b) stress profile.
Applsci 11 03649 g007
Figure 8. Divisions of the confined concrete: (a) exact divisions; (b) simplified divisions.
Figure 8. Divisions of the confined concrete: (a) exact divisions; (b) simplified divisions.
Applsci 11 03649 g008
Figure 9. Enhancement of lateral load capacity: (a) ALR = 0.15; (b) ALR = 0.3.
Figure 9. Enhancement of lateral load capacity: (a) ALR = 0.15; (b) ALR = 0.3.
Applsci 11 03649 g009
Figure 10. Reinforcement details of column: (a) front view; (b) plane view.
Figure 10. Reinforcement details of column: (a) front view; (b) plane view.
Applsci 11 03649 g010
Figure 11. Strengthened RC column: (a) front view; (b) plane view.
Figure 11. Strengthened RC column: (a) front view; (b) plane view.
Applsci 11 03649 g011
Table 1. Range of four variables in parametric study.
Table 1. Range of four variables in parametric study.
tp (mm)ALRdc (mm)ρl
3, 4, 50.15, 0.3400, 5000.015, 0.03
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Shan, Z.; Chen, L.; Liang, K.; Su, R.K.L.; Xu, Z. Strengthening Design of RC Columns with Direct Fastening Steel Jackets. Appl. Sci. 2021, 11, 3649. https://doi.org/10.3390/app11083649

AMA Style

Shan Z, Chen L, Liang K, Su RKL, Xu Z. Strengthening Design of RC Columns with Direct Fastening Steel Jackets. Applied Sciences. 2021; 11(8):3649. https://doi.org/10.3390/app11083649

Chicago/Turabian Style

Shan, Zhiwei, Lijie Chen, Kun Liang, Ray Kai Leung Su, and Zhaodong Xu. 2021. "Strengthening Design of RC Columns with Direct Fastening Steel Jackets" Applied Sciences 11, no. 8: 3649. https://doi.org/10.3390/app11083649

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop